We use cookies to improve your browsing experience, but also to analyze our traffic. By clicking “Accept All”, you consent to our use of cookies.
We use cookies to help you navigate efficiently and perform certain features. You will find detailed information about all cookies under each consent category below.
We also use third-party cookies that help us analyze how you use this website. These cookies will only be stored in your browser with your prior consent.
You can choose to enable or disable some or all of these cookies, but disabling some of them may affect your browsing experience.
Material category
Austénitique
Sectors of activity
Caractéristiques de la norme EN 10250-4, forgés ép. 250 mm max.
C
0.030 max %
Si
1.00 max %
Mn
2.00 max %
P
0.045 max %
S
0.030 max %
N
0.12-0.22 %
Cr
16.50-18.50 %
Mo
2.00-2.50 %
Ni
10.00-12.00 %
Rp0.2 min
280 min MPa
Rp0.2 max
0 MPa
Rm min
580-800 MPa
Rm max
0 MPa
A min
30 min transv %
Dureté max
0 HB
Résilience
100 long / 60 transv min J
Masse volumique
8.0 g/cm³
EN(num.)
1.4406
EN(sym.)
X2CrNiMoN17-11-2
ISO
-
NF
EN10028-7, EN10088-3, EN10222-5, EN 10250-4
UNI
-
DIN
17445
JIS
SUS316LN
SAEASTM
A182 F316LN
UNS
S31653
BS
316S61
AFNOR
Z3CND17-11Az, NF A 35-573
AISI
316LN
Autres
AISI 316LN